Shoutout to the painter at our shop who showed me I was blocking primer way too early
I kept getting sand scratch swelling on dark colors and figured it was the gun or my air pressure. He pointed out I was wet sanding my primer with 600 grit only 40 minutes after spraying, while the shop was sitting at 61 degrees. Once I started waiting a full day and hitting it with 400 first, the swelling went away on a black Silverado I did in Fayetteville. Felt pretty dumb but it saved me a respray. How long do you all let primer cure when the booth is cold like that?
Temperature swings overnight mess with cure way more than the cold itself. Primer keeps crosslinking while it cools, so if you sand at 40 minutes in a 61 degree shop and it drops to 55 overnight, you already broke the skin before it finished. Watching the temp curve, not the clock, is what got me past this.